• Process condition for Insulation Board product
Grade
Density
(g/l)
Pre-expansion
Optimum aging time
B/M molding
Drying
(Day)
Cutting
steam
charge
(kg/§²)
expan-
sion ratio
Winter season
Summer season
steam charge (kg/§²)
1st steam
2nd steam
Wire
thick-
ness
(mm)
Pressure
(kg/§²)
Time(s)
Pressure
(kg/§²)
Time(s)
SE-1600
20~25 0.25
 ~
0.30
40~50
24~30
20~26
2.0
~
3.0
0.52
10
~
13
0.62
2
~
3
3
~
4
0.3
~
0.5
17~20
50~59
18~24
14~20
0.57
0.67
14~17
59~71
12~18
8~14
0.62
0.72
SE-2000
25~30
33~40
24~30
20~26
0.50
0.60
20~25
40~50
18~24
14~20
0.55
0.65
15~20
50~67
12~18
8~14
0.60
0.70
12~15
67~83
6~12
4~8
0.65
0.75
SE-2500
25~30
33~40
20~30
15~20
0.55
0.65
20~25
40~50
14~20
10~15
0.60
0.70
15~20
50~67
8~14
6~10
0.65
0.75
13~15
67~77
4~8
3~6
0.70
0.80
SE-3000
30~40
25~33
20~30
15~20
0.55
0.65
25~30
33~40
14~20
10~15
0.60
0.70
20~25
40~50
8~14
6~10
0.65
0.75
15~20
50~67
4~8
3~6
0.70
0.80

 
SH Energy Bldg. 9F, 16-6, Sunae-dong, Bundang-gu, Seoul, Korea
Tel : (031) 8022 - 0700 Fax : (031) 8022 - 0783 Mail : webmaster@sh-enerchem.com
Copyright(C) 2000 SH Energy & Chemical Co., Ltd. All Right Reserved.